Within the scope of the "The Effect of Ca-Si Inoculant on Mechanical Properties" project, the effects of a Ca-Si based inoculant — as an alternative to the La-based inoculants used in the production of EN-GJS-600-3 (GGG-60) grade ductile iron — on microstructure, mechanical properties, wear behavior and machinability were comprehensively investigated and successfully completed. In the study, stepped test blocks with section thicknesses of 5, 15, 25, 35 and 50 mm were produced by conventional sand casting in order to reveal the influence of different cooling rates and section thicknesses; three inoculation conditions, namely 0.2% La-based, 0.2% Ca-Si based and 0.1% Ca-Si based, were evaluated comparatively. On the samples obtained, microstructural parameters such as nodule count, nodularity, graphite nodule size and distribution and the ferrite/pearlite ratio were examined together with Brinell hardness, yield and tensile strength, elongation at fracture, wear behavior and machinability, thus revealing the relationship between the type and amount of inoculant and the performance of the material. As a result of the project, the effectiveness of the Ca-Si based inoculant in achieving the targeted microstructural and mechanical properties at different section thicknesses was evaluated and the applicability of a lower-cost inoculation approach in ductile iron production was demonstrated. Compared with the cost of the La-based inoculant of approximately 2,500 USD/ton, the Ca-Si based inoculant costs approximately 1,500 USD/ton and can be used at lower addition rates, which is expected to provide significant savings in inoculation costs and thereby reduce final casting part costs. The project has produced an important R&D output for evaluating alternative raw materials and process parameters in high-performance ductile iron production, reducing production costs and increasing resource efficiency.

Brinell Hardness Values by Section Thickness

SectionBa-based inoculantCa-Si half additionCa-Si full addition
Thickest149.7 HB154.6 HB152.9 HB
Thick152.3 HB154.3 HB142.1 HB
Thin156.8 HB157.9 HB152.8 HB
Thinnest147.2 HB153.7 HB150.3 HB

Tensile Test Results

InoculantSampleFm (kN)Rm (N/mm²)Rp0.2 (N/mm²)Elongation (%)E Modulus (GPa)Test Speed (mm/min)
Ba-based inoculant112.471635.26396.4611.452.327
Ba-based inoculant212.486636.02392.288.022.335
Ca-Si half addition112.931658.69400.1317.60.125
Ca-Si half addition213.218673.31401.7611.212.455
Ca-Si full addition113.921709.12322.8513.60.065
Ca-Si full addition213.551690.27400.5812.65.155